a) Tabela pomiarów i obliczeń
Lp. |
Materiał badany |
Grubość badanej płytki |
Skrośna |
Powierzchniowa |
|||||||||||
|
|
|
RV1 |
RV2 |
Ab |
ၲv |
RS1 |
RS2 |
Ab |
ၲs |
|||||
|
|
h1 |
h2 |
h3 |
hśr |
15s |
60s |
|
15s |
60s |
15s |
60s |
|
15s |
60s |
|
|
[mm] |
[mm] |
[mm] |
[mm] |
[Gၗ] |
[Gၗ] |
- |
[ၗcm] |
[ၗcm] |
[Gၗ] |
[Gၗ] |
- |
[ၗ] |
[ၗ] |
1 |
Płyta papierowo ftalowa PcF |
0,33 |
0,33 |
0,33 |
0,33 |
3,372 |
3,552 |
1,05 |
260,743 |
274,662 |
0,33 |
0,33 |
0,33 |
8,442 |
8,442 |
2 |
Płyta papierowo fenylowa TcF |
0,5 |
0,51 |
0,5 |
0,503 |
0,02061 |
0,02003 |
0,97 |
1,045 |
1,015 |
2,467 |
2,467 |
1 |
63,110 |
63,110 |
3 |
Szkło |
3,06 |
3,37 |
3,36 |
3,263 |
5,741 |
6,278 |
1,09 |
44,892 |
49,091 |
1,959 |
2,324 |
1,18 |
50,114 |
59,451 |
4 |
Porcelana |
5,31 |
5,47 |
5,45 |
5,41 |
148 |
226,9 |
1,53 |
698,078 |
1070,229 |
61,42 |
60,47 |
0,98 |
1571,218 |
1546,916 |
5 |
Poliuretan |
2,14 |
2,12 |
1,93 |
2,063 |
0,04696 |
0,04696 |
1 |
0,581 |
0,581 |
3,666 |
3,636 |
0,99 |
93,782 |
93,014 |
6 |
Preszpan |
1,07 |
1,06 |
1,02 |
1,05 |
0,02575 |
0,02542 |
0,98 |
0,626 |
0,618 |
0,7757 |
0,7865 |
1,01 |
19,844 |
20,120 |
7 |
Polietylen |
0,2 |
0,19 |
0,19 |
0,193 |
313,6 |
670,4 |
2,13 |
41391,285 |
88484,430 |
>1100 |
>1100 |
- |
>28139,69 |
>28139,69 |
8 |
Elastometr silikonowy bez wypełniacza |
3,02 |
3,01 |
3 |
3,01 |
>1100 |
>1100 |
- |
>9325,364 |
>9325,364 |
>1100 |
>1100 |
- |
>28139,69 |
>28139,69 |
W przypadku, kiedy nie można było odczytać wartości rezystancji skrośnej (np. dla elastometru silikonowego bez wypełniacza), przyjmowaliśmy maksymalną wartość katalogową, jaką był w stanie zmierzyć miernik, równą 1,1TΩ. Rzeczywista wartość rezystancji skrośnej przekraczała wartość 1,1TΩ.
Ab - współczynnik absorpcji równy
Wszystkie pomiary były wykonywane przy napięciu 1kV