Protokół
Laboratorium Inżynierii Materiałowej nr 3
Badanie podstawowych własności magnetycznych materiałów ferromagnetycznych.
Schemat układu pomiarowego.
Ferryt.
Vx |
Vy |
R1 |
R2 |
N1 |
N2 |
C |
S |
LŚR |
V/cm |
V/cm |
Ω |
Ω |
|
|
μF |
m2 |
m |
|
|
|
|
|
|
|
|
|
Tabela pomiarów:
L.p. |
f |
Bm |
Hm |
Bk |
Hk |
Bm |
Hm |
Bk |
Hk |
|
Hz |
dz |
dz |
dz |
dz |
T |
A/m |
T |
A/m |
1 |
1,3kHz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
1 |
1,8kHz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
Vx |
Vy |
R1 |
R2 |
N1 |
N2 |
C |
S |
LŚR |
V/cm |
V/cm |
Ω |
Ω |
|
|
μF |
m2 |
m |
|
|
|
|
|
|
|
|
|
Tabela pomiarów:
L.p. |
f |
Bm |
Hm |
Bk |
Hk |
Bm |
Hm |
Bk |
Hk |
|
Hz |
dz |
dz |
dz |
dz |
T |
A/m |
T |
A/m |
1 |
70Hz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
1 |
100Hz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
Blacha na podwyższone częstotliwości.
Vx |
Vy |
R1 |
R2 |
N1 |
N2 |
C |
S |
LŚR |
V/cm |
V/cm |
Ω |
Ω |
|
|
μF |
m2 |
m |
|
|
|
|
|
|
|
|
|
Tabela pomiarów:
L.p. |
f |
Bm |
Hm |
Bk |
Hk |
Bm |
Hm |
Bk |
Hk |
|
Hz |
dz |
dz |
dz |
dz |
T |
A/m |
T |
A/m |
1 |
100Hz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
1 |
130Hz |
|
|
|
|
|
|
|
|
2 |
|
|
|
|
|
|
|
|
|
3 |
|
|
|
|
|
|
|
|
|
4 |
|
|
|
|
|
|
|
|
|
5 |
|
|
|
|
|
|
|
|
|
6 |
|
|
|
|
|
|
|
|
|
Strona 1 z 2