Schichtdicke 30 pm, 400 W131 |
Wie gębaut |
Warmebehandełt1131 | ||
Layer thickness 30 pm, 400 W131 |
As-built |
Heat-treated1131 | ||
M: Mittelwert Mean SD: Standardabweichung Standard deviation |
M |
SD |
M |
SD |
Zugpriifung!10! Tensile test1105
Zugfestigkeit Tensile strength |
RJMPa] |
0° 45° 90° |
473 479 482 |
15 15 15 |
257 265 264 |
10 10 10 |
Dehngrenze |
R^tMPa] |
0° |
305 |
2 |
152 |
5 |
Offset yield strength |
45° |
290 |
5 |
155 |
4 | |
90° |
276 |
5 |
150 |
6 | ||
Bruchdehnung |
A [%] |
0° |
7 |
2 |
12 |
5 |
Elongation at break |
45° |
6 |
2 |
12 |
5 | |
90° |
5 |
2 |
11 |
5 | ||
BrucheinschnUrung |
Z[%] |
0° |
10 |
2 |
46 |
4 |
Reduction of area |
45° |
7 |
2 |
37 |
2 | |
90° |
7 |
2 |
37 |
2 | ||
Elastizitatsmodul |
E [GPa] |
0° |
77 |
4 |
58 |
5 |
Young's modulus |
45° |
71 |
5 |
63 |
12 | |
90° |
75 |
3 |
52 |
4 |
Harteprufung1”1
Hardnesslest1"1