INDICATOR |
TESTING RESULT |
METHODOLOGY |
ADDITIONAL INFORMATION |
Fastness to abrasion |
PN-EN ISO |
Load -12 kPa; | |
[No. of strokes] |
12947-2:2000+AC:2006 |
Eraser: a standard wool cloth, | |
sample 1 |
25.000 |
A foam pad was used in the handles; | |
sample2 |
25.000 |
A magnifying device with the magnification ratio of 8; | |
sample 3 |
25.000 |
Testing bracket: 5.000 strokes; | |
sample 4 |
25.000 |
Notę: | |
average fastness to abrasion |
>20.000 |
It was not observed that the sample had been worn thro-ugh after 25.000 strokes. The testing ended after the number of strokes as agreed on with the customer. | |
Oleophobicity |
PN-EN ISO | ||
sample 1 |
5.5 |
14419:2010 | |
sample 2 |
5.5 | ||
sample 3 |
5.5 | ||
the degree of oleophobicity |
5.5+0.5 | ||
Fastness to rain |
PN-91/P-04629 |
Rain for: 5 minutes | |
Absorbability [%] |
8.3+1.7 | ||
Water permeability [cm3] |
0.90 | ||
Color fastness to friction |
PN-EN ISO |
Mandrel: 016mm; | |
105 X12:2005 |
force: 9 N | ||
the whiteness soiled to the fol-lowing degree dry along + across |
4+4 | ||
Color fastness to alkaline t acid |
PN-EN ISO |
Temperaturę: -60°C; | |
sweat [degree] |
105-C06:2010 |
method: - CIS; 25 Steel balls were used. | |
change to the color of the sample |
4/5 | ||
the whiteness soiled PES fabric |
4/5 | ||
the whiteness soiled CO fabric |
4/5 |
INDICATOR |
TESTING RESULTS |
TESTING METHOD AS PER | |
Raw materiał composition [%] |
Expressed in the sample dry weight |
Taking into account hu-midity allowances |
PN-72/P-04604 |
Cotton 52.9% Polyester 47.1% |
Cotton 54.5% Polyester 45.5% |
PN-93/P-04847.10 | |
The pH of water extract Type of solution used - water, t = 21.4°C, pH = 7.1 |
7.4 |
PN-EN ISO 3071:2007 | |
The content of free formaldehyde [mg/kg] |
not detected |
PN-EN ISO 14184-1:2011 | |
Sample mass: 2.5 g Curve rangę: 16.5-660 ppm |
Person authorizing laboratory test results
Legible signature/stamp